Start with 1.00 mm HDPE (about 40 mil) for a grow-out shrimp pond with a smooth, prepared base and suitable liner protection. Consider 0.75 mm (about 30 mil) for a small, shallow nursery pond with a smooth base and little traffic. For rocky ground, a concrete sump or frequent maintenance access, compare 1.25 and 1.50 mm with a protection plan. These are starting points for a quote, not design minimums.
Thickness by pond condition
| Pond condition | Starting grade | Check before ordering |
|---|---|---|
| Small nursery pond | 0.75 mm (≈30 mil) | Confirm that the base is smooth, the liner is protected and routine traffic is limited. |
| Grow-out pond | 1.00 mm (≈40 mil) | Check protection at aerator supports, harvest routes and drains. |
| Rocky base, concrete sump or frequent access | Compare 1.25 and 1.50 mm (≈50 and 60 mil) | Check the prepared base, cushion, hard edges and equipment loads. Do not assume machinery can drive on the liner. |
| Steep banks | No thickness from slope alone | Check stability and interface shear resistance before choosing the liner surface and thickness. |
Millimetre and mil grades are nominal pairings, not exact conversions. One mil is 0.0254 mm: 30, 40, 50 and 60 mil are exactly 0.762, 1.016, 1.270 and 1.524 mm, respectively. Write the controlling unit on the order. [1]
Is 20 mil enough? It converts to 0.508 mm. A nominal 0.50 mm or 20 mil sheet falls below the scope of GRI-GM13 Revision 19 (June 11, 2025), which covers smooth and textured HDPE from 0.75 to 3.00 mm (nominally 30 to 120 mil). Do not treat 20 mil as equivalent to 30 mil. GRI-GM13 sets manufacturing requirements, not shrimp-pond design thicknesses. [2]
What thicker HDPE buys
Moving from 1.00 to 1.25 mm raises the smooth-sheet minimum average for index puncture from 320 to 400 N. At 1.50 mm it is 480 N. Use those figures to compare material grades, not to assign an allowable load to an aerator foot or a vehicle tire. [2]
| Property | 0.75 mm | 1.00 mm | 1.25 mm | 1.50 mm |
|---|---|---|---|---|
| Puncture, ASTM D4833 | 240 N | 320 N | 400 N | 480 N |
| Tear, ASTM D1004 | 93 N | 125 N | 156 N | 187 N |
| Tensile yield, ASTM D6693 | 11 kN/m | 15 kN/m | 18 kN/m | 22 kN/m |
| Tensile break, ASTM D6693 | 20 kN/m | 27 kN/m | 33 kN/m | 40 kN/m |
| Lowest individual thickness | 0.675 mm | 0.90 mm | 1.125 mm | 1.35 mm |
Smooth sheet is measured by ASTM D5199: the minimum average is the nominal grade, and the lowest of 10 readings may be no more than 10% below nominal. Textured sheet uses ASTM D5994 for core thickness. The minimum average is 95% of nominal; at least eight of 10 readings must be at least 90%, and none may be below 85%. Where weld edges are present, modified D5199 applies, with a 90% individual minimum. GRI-GM13 lists a minimum average texture height of 0.40 mm in its metric table (ASTM D7466). [2] [3] [4]
GRI-GM13 uses ASTM D6693 Type IV for tensile testing. For the four smooth grades shown, the minimum average elongation is 12% at yield and 700% at break, and the stress-crack requirement is 500 hours under the ASTM D5397 appendix test. Textured sheet has its own requirements: at 1.00 mm, for example, the index puncture minimum average is 267 N, not 320 N. Select a textured HDPE liner based on the interfaces in the slope design, not on the texture height or sheet thickness alone. [2] [5]
Checks that can change the grade
FAO guidance on shrimp-pond design calls for an even bottom free of projecting rocks and stumps. If sharp material remains, have the designer specify how to prepare the base and whether to use a protective geotextile cushion. A thicker sheet is not a substitute for either check. [6]
Example: comparing two grow-out quotes. Suppose one pond has a smooth base and protected aerator supports, while the other has a concrete sump and a harvest route across the lined floor. Use 1.00 mm as a quote baseline for the first. For the second, ask for the sump transition, pipe seal and harvest-route protection to be shown on the liner plan before comparing 1.25 and 1.50 mm. If one quote omits those details, the two prices do not cover the same work.
Depth alone does not tell you which sheet to buy. At 1.5 m depth, static freshwater pressure is about 14.7 kPa using a density of 1,000 kg/m³ and gravity of 9.81 m/s². That pressure is not directly comparable with sheet tensile values in kN/m. During drawdown, check groundwater uplift and whether the design needs drainage or venting beneath the liner. [7] [8]
What to verify on the quote
- Roll identification. Specify the nominal HDPE liner thickness, surface and acceptance method. Ask for test records traceable to the supplied rolls. GRI-GM13 specifies a minimum average formulated density of 0.940 g/cm³ (ASTM D1505 or D792). At that assumed density and nominal thickness, 1.00 mm is about 0.94 kg/m² and 1.50 mm is about 1.41 kg/m², excluding overlaps and packaging. [2]
- Weathering. For exposed liner, ask for formulation records covering carbon black content (2.0–3.0%, ASTM D4218 or a correlated method), dispersion (ASTM D5596) and oxidative induction time (OIT). GRI-GM13 lists minimum averages of 100 minutes for standard OIT (ASTM D8117) or 400 minutes for high-pressure OIT (ASTM D5885). After oven aging at 85°C for 90 days (ASTM D5721), the applicable minimum average retention is 55% or 80%, respectively. Its UV criterion is at least 50% average high-pressure OIT retention after 1,600 hours under ASTM D7238, cycling 20 hours of UV at 75°C and four hours of condensation at 60°C. This is a lab criterion, not a service-life estimate. [2]
- Water contact. Request written suitability for the exact formulation at your operating salinity and temperature, plus compatibility with the planned cleaners or disinfectants at their intended concentrations and contact times. A thickness label is not a compatibility rating. If the design requires a numerical permeation or seepage limit, request the applicable test method and supporting data rather than inferring a value from thickness.
- Seams and penetrations. Specify a panel layout, drain and pipe details, and acceptance criteria for the field seams. Choose nondestructive checks for the seam type and specify destructive peel and shear sampling under ASTM D6392 for applicable thermofusion seams. The test method is not a project pass limit. [9]
Have qualified personnel confirm the final liner design, installation and inspection under local rules. Before filling, ask them to confirm that the installed protection, sump details and seam records match the approved plan.