If testing traces the leak to the area of a geomembrane seam, look for an incompletely bonded weld, a gap at a T-joint or extrusion start, or a tear in the sheet beside the weld. But if the only result was a drop in water level, you have not shown that the seam failed. First check the test setup and locate where water crosses the containment barrier. The spot where it shows up may not be the source.
Check what the test actually measured
For a pond or tank fill test, compare the recorded water level, test head and hold time with the approved procedure. Check the measurement setup, valves, plugs, drains and penetrations before blaming the liner. Account for rainfall, evaporation or temperature effects as the procedure requires. A test run outside the specified conditions does not establish whether the seam meets the acceptance criteria.
Example: Suppose seepage seen near the crest during filling disappears after the water level falls. Record the water levels at which seepage started and stopped, and check nearby seams or fittings at those elevations. The change helps narrow the search but does not rule out a defect lower down, where the water pressure also dropped. A dry inspection at the lower level is not a pass at the specified head.
If a lab applied water pressure to a seam specimen, use the leak criterion in that test procedure. If the report instead records an air-channel, vacuum chamber or peel and shear test, interpret it for what it measures:
- Air-channel test: ASTM D5820 checks the continuity of a dual-track seam by pressurizing the channel between its weld tracks. It does not measure weld strength [1].
- Vacuum chamber test: ASTM D5641 uses bubbles to identify a local leak path. The chamber has to seal over the area being checked [2].
- Peel and shear testing: ASTM D6392 evaluates specimens cut from thermally bonded, nonreinforced geomembrane seams. A passing specimen does not prove the entire seam is leak-free [3].
Have qualified personnel choose and perform the tests, interpret the results and carry out any repairs under the project specification and applicable local requirements.
Read the HDPE seam strength report
If the project specifies GRI-GM13 Revision 19 (June 11, 2025), use Section 6.2 and Table 3(b) to check the metric limits for thermally bonded smooth and textured HDPE seams. These are specimen acceptance limits, not averages, design values or hydrostatic pass criteria. Do not apply them to LLDPE liners [4].
| Nominal thickness | Shear, both methods | Hot-wedge peel | Extrusion-fillet peel |
|---|---|---|---|
| 1.0 mm | 350 | 263 | 225 |
| 1.5 mm | 525 | 398 | 340 |
| 2.0 mm | 701 | 530 | 455 |
All five specimens in each test mode must meet the applicable strength minimum and have acceptable break patterns. For peel, separation cannot exceed 25% of the original bonded area on any specimen. In laboratory shear testing, elongation at break must be at least 50%; the table note omits elongation measurements for field testing. A break pattern helps interpret the result, but does not by itself identify a welding error [4].
Worked example: On a 1.5 mm hot-wedge HDPE seam, suppose four peel specimens reach 410 N per 25 mm and one reaches 390. The average is 406, above the 398 minimum, but the sample does not meet the GRI-GM13 strength criterion because one specimen fell short. If that fifth specimen instead reaches 410 but shows 30% peel separation, it still does not meet the separation limit. Ask for the individual readings and break patterns, not just the average or the pass/fail label [4].
Trace the leak before choosing a repair
- Along a straight weld: Check for dirt or moisture trapped in the overlap and compare the production log with the approved trial weld. Review heat, speed and pressure together; a weak peel result does not identify the cause on its own. Use the roll tags and material traceability records to verify the sheet type, thickness and whether the sheet is textured or smooth.
- At a T-joint, weld start or pipe boot: Inspect the transition for a gap where the sheets step up or an extrusion bead starts or stops. Check the detail separately; a passing result on the straight run does not clear the intersection. Compare the pipe boot and its seals with the approved drawings.
- Beside the weld: Look for a cut, puncture or tear, especially where the sheet spans a low spot or is pulled tight. For liners covered by water or earthen material, ASTM D7007 describes electrical leak location methods that can help distinguish sheet damage from a seam defect when survey conditions are suitable [5].
Field example: Suppose a dual-track air-channel test passes, but seepage appears below a pipe boot during filling. Mark the wet spot on the panel drawing, then check the boot weld and adjacent sheet rather than reopening the straight seam. If a vacuum chamber cannot seal around the boot, a qualified tester can consider ASTM D6365 spark testing if the detail is suitable and the quality plan allows it [6].
When the air-test report looks good but coverage is unclear: Check whether the tester recorded a pressure drop at the gauge when the far end of the channel was opened. Pressure can hold on the gauge side of a blockage even though the rest of the run was not tested. If the far-end check was required but is missing or inconclusive, ask the tester to verify the actual coverage and follow the quality plan for any unverified section [7].
Repair and retest the affected area
An isolated defect may call for a patch; a longer poorly bonded run may need replacement. If the liner bridges a low spot, have the project team address the support problem before rewelding. Use the approved repair detail and the retest method and acceptance criteria specified for the repaired geometry. An extrusion patch, for example, does not necessarily have an air channel to retest. If the project also requires a repeat fill test, a local repair check does not replace it.
Set the repair limits before cutting. A failed peel sample identifies a problem at the sampled location, not the length of seam affected. Where the quality plan calls for additional samples, have the quality assurance team locate passing results in both directions. If the first follow-up passes on one side but fails on the other, the failed side is still unbounded. Patching the original sample hole does not close out the weak run [7].
In the as-built seam and test records, tie the seam ID and repair limits to the panel drawing, original test, repair method and retest result. Before covering or resuming filling, confirm which items the quality plan requires the project team to release: the local repair, the original failed seam test, and any repeat fill test. To prevent a repeat, keep overlaps clean and dry, check that trial welds represent production conditions, and agree in advance how T-joints, patches and penetrations will be tested.
Need the liner details for a seam review?
Share the liner type, thickness, seam layout and test method with Jinseed when requesting product information for your project team.