Yes, but only if the panels stay stable, both faces of the overlap stay clean and dry until welding, and a trial seam passes peel and shear tests under the conditions you will weld in. If gusts move the panels or dust returns after cleaning, stop. A trial seam that passed earlier does not override a stop-work limit or qualify welding under changed conditions.
Qualified personnel must carry out welding and testing under the approved construction quality assurance (CQA) plan, site safety procedures, and applicable local regulations. Use the project’s limits for wind and sheet temperature rather than a generic wind-speed cutoff.
When to stop welding and what to check before restarting
| What you see on site | What to do |
|---|---|
| Panels stay in position, the overlap stays clean and dry, and the trial seam passes. | Start production only within the approved weather and operating limits. |
| Gusts lift a panel edge, shift the overlap, or exceed the site limit. | Stop. Follow the approved panel-control procedure. Recheck alignment and qualify the setup in the new conditions before restarting. |
| Dust settles on either mating face before it reaches the welder. | Stop and clean both faces. Reduce the length of overlap exposed at one time or use approved shelter. If the faces will not stay clean, wait. |
| A wrinkle or fishmouth prevents the faces from lying flat. | Hold that section and correct the fit using the approved procedure before welding. |
| A trial fails in peel or shear. | Hold production, correct the cause, and pass a new trial before restarting. |
| A production seam has no accepted test record. | Keep it exposed until the required tests are complete and any failures are resolved. |
What to confirm before the shift
- Weather limits and who can restart work. Check whether the site limit is based on gusts, an average, or both, where readings are taken, and who clears the restart. A sheltered reading does not settle whether an exposed seam meets the limit.
- What the trial must represent. Record the sheet temperature at the work area and distinguish it from air temperature and the welder setting. Confirm which changes in weather, sheet temperature, material, operator, machine, or settings trigger a new trial under the plan. If the next seam is on an exposed slope, do not assume that a passing trial made behind a windbreak qualifies it.
- How to find a seam again. Agree on how the crew will identify panels, seam IDs, and the start and stop locations. If a dust plume interrupts a pass, the CQA team needs to find the affected length later, not just know which shift welded it.
Keep both faces of the overlap clean
On a dusty pad, shorten the section you uncover and inspect both mating faces immediately before the pass. If dust settles again before the welder reaches that section, cleaning farther ahead will not solve the problem. GRI GM9, a cold-weather seaming practice, requires the seam area to be free of soil particles and other foreign matter and notes that movable enclosures can help at high-wind sites. It does not set a wind limit or a trial frequency for dusty sites[1].
Field example: A haul road becomes an upwind dust source
Suppose a crew passes its morning trial, then the wind shifts and haul trucks start blowing dust across the overlap. The upper face looks clean, but there is grit on the underside of the flap. The crew stops, marks where the conditions changed, and flags any seam length welded since that point for CQA review. The morning trial does not establish that the exposed length is sound.
Before restarting, the crew moves the cleaning point closer to the welder and uncovers a shorter length. It makes and tests a new trial with the production material, operator, equipment, and settings under the conditions at the seam. Even after the trial passes, it checks both faces of the production overlap just before the pass. If grit still returns after cleaning, the crew waits. The log ties the new trial result and restart location to the affected seam IDs. If the log cannot establish where the dust first reached the seam, the crew records the uncertainty and leaves the hold boundary to CQA.
Choose the welding method by seam geometry
| Method | Where it fits | What to watch in dust |
|---|---|---|
| Dual-track hot wedge | Long panel seams where the welder can track a stable overlap | Expose only the overlap the crew can keep clean ahead of the welder. |
| Extrusion welding | Approved details and repairs where a wedge cannot track | Keep the prepared surface clean between abrasion and welding. |
Switching methods does not make a contaminated surface weldable. See the guide to hot-wedge and extrusion seaming for how the two methods differ.
Trial seams and production seams answer different questions
Trial seams: Check the setup
A trial seam checks whether the current setup can produce an acceptable joint. ASTM D6392-25 describes destructive peel and shear testing for nonreinforced thermofusion seams[2]. Peel pulls the two faces apart at the bond; shear pulls the sheets in opposite directions along the plane of the seam. Use the test edition and criteria specified for the project.
Read the failure description as well as the force values. If the project adopts GRI GM19a, select the HDPE criteria for the actual sheet thickness and weld method. The specification addresses strength, shear elongation, peel separation, and where the specimen breaks[3]. For example, if the force meets the minimum but the bond separates beyond the permitted amount in peel, the trial still fails. Keep production on hold, investigate the surface preparation and setup, and pass a new trial before restarting. The failed test alone does not identify dust as the cause.
Production seams: Verify the installed weld
Production seams still need inspection and the specified nondestructive tests. For example, use the approved air-channel pressure test for applicable dual-track seams and an approved method such as vacuum-box testing where the geometry permits. A passing air-channel test is not a peel or shear result. Take destructive production samples at the frequency set by the CQA plan and keep any section represented by a failed sample on hold until its extent, repairs, and retest results have been resolved under that plan.
Suppose a dual-track seam holds pressure, but a destructive sample from that seam fails in peel. Record both results and keep the affected length uncovered. A new trial may qualify the setup for the next weld, but it cannot release the earlier length. The CQA plan governs how to locate the affected section and what repairs, tests, and records are needed to release it.
If the hot-wedge welder records temperature, travel speed, and pressure, match that trace to the seam ID and interruption location. GRI GM32 describes continuous recording of those three variables for production hot-wedge seams[4]. A trace can help investigate a change in settings, but it does not show whether dust reached the overlap. Keep the field observations and seam-test results with it.
Check the HDPE sheet separately from the seam
On a heap leach pad, seam acceptance does not establish chemical compatibility with the leach solution or confirm that the liner has the specified protection against loads. Check the grade against the approved design and actual solution chemistry, concentration, temperature, and exposure duration. Use the design to confirm the drainage aggregate and any protective cushion geotextile. The mining liner applications and heap leach pad liner guide explain where those checks fit into the system.
GRI GM13 Rev. 19 covers smooth and textured HDPE geomembrane from 0.75 to 3.0 mm, with a minimum average formulated density of 0.940 g/cm³. The two smooth-sheet thicknesses below are examples from Table 1(b), not design recommendations or field seam acceptance values[5].
| Property | 1.5 mm | 2.0 mm | ASTM method |
|---|---|---|---|
| Yield strength | 22 kN/m | 29 kN/m | D6693 Type IV |
| Break strength | 40 kN/m | 53 kN/m | D6693 Type IV |
| Tear resistance | 187 N | 249 N | D1004 |
| Puncture resistance | 480 N | 640 N | D4833 |
For smooth sheet, GM13 Table 1(b) gives a minimum average thickness equal to nominal and allows no individual reading among ten to fall more than 10% below nominal. In the textured area, Table 2(b) requires an average of at least 95% of nominal thickness; at least eight of ten readings must be at least 90% of nominal, and none may fall below 85%. Where smooth weld edges are provided on textured sheet, the standard evaluates their thickness separately[5].
For example, on a 2.0 mm textured roll covered by Table 2(b), the textured area needs an average of at least 1.90 mm, at least eight readings of 1.80 mm or more, and no reading below 1.70 mm. These are calculated minimums, not field measurements. An average of 1.90 mm alone does not establish that the roll meets the point limits or that the weld edges meet their separate requirement[5]. Confirm the grade and weld-edge detail for the specified HDPE liner or textured geomembrane, and keep the batch documentation with the roll and seam records.
GM13 also lists a carbon black range of 2.0–3.0%, minimum average standard oxidative induction time (OIT) of 100 minutes or high-pressure OIT of 400 minutes, and 500 hours of stress-crack resistance under ASTM D5397 Appendix. For textured sheet, the stress-crack specimens come from smooth roll edges or smooth sheet of the same formulation[5]. GRI GM10 describes the single-point notched constant tensile load (SP-NCTL) test[6].
The GM13 oven-aging thresholds are 55% standard OIT retention or 80% high-pressure OIT retention after 90 days at 85°C. The UV threshold is 50% high-pressure OIT retention after 1,600 hours under ASTM D7238, with cycles of 20 hours of UV at 75°C followed by 4 hours of condensation at 60°C. Use these laboratory criteria to check the specified sheet formulation, not to predict service life or approve a field seam[5].
Specifying an HDPE liner for a heap leach pad? Share the required thickness, surface finish, and weld-edge details to discuss liner options and batch documentation.